WhatsApp
By Marcus Somadjaja

The quiet fix that powers copper and gold: electrolyte cleanup before electrowinning

  • beta-pramesti-asia
  • industry-gold-dan-copper-mining
  • process-electrowinning

The quiet fix that powers copper and gold: electrolyte cleanup before electrowinning

High-purity electrolyte makes or breaks electrowinning. Mines are doubling down on solvent extraction, targeted precipitation, and disciplined bleed streams to keep impurities in check — and current efficiency high.

Industry: Gold_&_Copper_Mining | Process: Electrowinning

Electrowinning (EW, electrodeposition of metal from solution) thrives on clean chemistry. Even trace impurities in the electrolyte can dent current efficiency, pit cathodes, or spark toxic by-products. Copper circuits lean on solvent extraction (SX, transferring copper into an organic phase to separate it from contaminants); gold circuits lean on precipitation. Both ultimately rely on a simple discipline: a regular bleed to stop what chemistry can’t catch.

The data are unambiguous. In copper SX–EW, solvent extraction is the primary purification step, selectively moving Cu into the organic phase and leaving most contaminants in the raffinate. Modern SX circuits routinely exceed 95% Cu recovery in stripping while co-extracting only a few percent of Fe, Zn, Ni and other metals (www.mdpi.com). On a complex feed, a single extraction stage (20% extractant, organic/aqueous ratio O/A 3, pH≈1.5) removed 88.1% of Cu with <8% co-extraction of Fe, Zn, Ni and Sn; optimized stripping (H₂SO₄ 180 g/L, O/A 2) then recovered 95.3% of Cu while limiting impurities passed to the electrowinning electrolyte to <6% (www.mdpi.com).

Yet the stubborn few — chlorides, nitrates, iron redox couples, and odd-trace metals like Sb or Bi — demand targeted moves before the electrolyte enters the cells.

Solvent extraction as primary purification

Well-designed SX yields a catholyte containing almost only copper, with most Fe, Al, and others left behind. But certain anions and metals need extra attention. High chloride (Cl⁻) or nitrate (NO₃⁻) in the pregnant leach solution (PLS, metal-bearing leach liquor) can follow copper into the electrolyte and either corrode stainless steel or generate chlorine gas at the anode. Chilean mines processing liquors with >30 g/L Cl add extra water-wash stages so catholyte Cl⁻ stays below ~30–50 mg/L (www.scielo.org.za) (blog.emew.com). The recommended chloride limit in copper EW feed is on the order of 50 ppm; above this, chlorine evolution and cathode pitting accelerate (blog.emew.com). Many SX plants therefore include a scrubbing or wash stage to purge halides (and nitrates) before the organic goes to strip (www.scielo.org.za).

Iron redox cycling and oxidative precipitation

Even small Fe in the catholyte undermines efficiency via the Fe²⁺/Fe³⁺ redox cycle. A typical guideline is to keep the Cu:Fe molar ratio >6:1; if the ratio falls below this, ferrous/ferric cycling can consume significant power (blog.emew.com). Accordingly, many circuits further polish the strip solution to remove Fe by oxidative precipitation: raising catholyte pH (with CaO/NaOH) in the presence of an oxidant (often O₂ or H₂O₂) precipitates Fe(III) as fibrous goethite (FeOOH) or jarosite compounds, eliminating >95% of Fe. In a zinc-electrowinning analog, Fe and As were removed by NaOH+H₂O₂ at pH≈3.5 (link.springer.com); this suggests similar goethite treatment would scrub Fe out of Cu electrolytes.

Precipitation steps depend on precise reagent addition. In practice, plants deploy accurate chemical dosing to hit pH and oxidant setpoints; for example, dosing can be managed with a dosing pump to meter NaOH or H₂O₂ during goethite/jarosite formation.

Targeted removal of trace metals

Some high-impurity ores (or recycling feeds) introduce trace elements like As or Sb. Laboratory studies have shown that Sb and Bi can be selectively extracted from Cu/HCl electrolytes using solvating organophosphorous solvents (www.nature.com). Alternatively, Ni and Co (if present) can often be precipitated as hydroxides by raising pH above 9–10, or removed by sulfide precipitation. In practice, the combination of SX plus targeted precipitation or ion-exchange keeps these impurities at sub-ppm levels in industrial electrolytes. Where ion exchange is specified, a plant-scale solution would be a cation/anion system such as an ion-exchange unit with appropriate resin selection.

Precipitation methods and cementation sequencing

Where SX is not used (or as a supplementary step), chemical precipitation is standard for impurity removal. Iron and arsenic: ferric iron is most efficiently removed by raising pH to ~3–4 under oxidizing conditions. Commercial copper refining has long used jarosite or goethite processes: e.g., adding K₂SO₄ and NaOH at 90–95 °C precipitates jarosite (KFe₃(SO₄)₂(OH)₆) and removes >90% of Fe. In one laboratory case, Fe (and As) were removed by NaOH+H₂O₂ to pH≈3.5 at essentially 100% efficiency (link.springer.com).

Copper, zinc, cadmium, aluminum: these can be removed by cementation or co-precipitation with other metals. Adding zinc dust at pH≈5 causes Cu²⁺, Cd²⁺ and Al³⁺ to plate or precipitate with Zn (as Zn²⁺ goes into solution) (link.springer.com). In zinc refineries, this step routinely cleans residual Cu/Cd/Al to trace levels, and a two-stage approach (first Fe/As at low pH, then Cu/Cd at higher pH) is recommended (link.springer.com). Especially in gold/cyanide (CN) circuits or mixed-metal leachates, adding sulfide (e.g., Na₂S, NaHS) at low pH selectively precipitates insoluble metal sulfides: treating the barren cyanide solution at pH≈3 with Na₂S removes over 99% of Cu²⁺, Zn²⁺, Fe²⁺ and Pb²⁺; in one experiment, “lead, zinc, copper and iron ions” were essentially completely removed (∼99% recovered in solids) by sulfide precipitation at pH 3–4 (file.scirp.org).

Hydroxide/carbonate precipitation: at high pH (9–11), hydroxides of many metals (Zn, Ni, Co, Mn, Fe) will precipitate. For example, adding Ca(OH)₂ (lime) to a cyanide solution raises pH and precipitates Zn(OH)₂ and Ni(OH)₂, removing those from solution. (No specific data available here, but typically >90% removal of soluble Zn/Ni at pH≥9.) In practice, removal efficiencies are very high when conditions are optimized. A two-stage precipitation pilot removed Pb, Zn, Cu, Fe to <1% of original by adjusting pH in steps (file.scirp.org). These processes produce solid sludges (e.g., jarosite, sulfides) that must be handled or recycled.

Solid-liquid separation is the practical companion to precipitation. Compact settlers such as a lamela settler offer the retention time and footprint fit needed to capture jarosite/goethite or metal sulfide sludges before electrolyte polishing.

Operating limits and electrolyte polishing

Industrial circuits keep impurity thresholds very low — for example, Fe at <~5 mg/L and Cl⁻ at <50 mg/L — to avoid current losses, corrosion or chlorine evolution (blog.emew.com) (blog.emew.com). With SX removing the bulk (Cu yield >90–95%; Fe, Zn, Ni pushed to raffinate) (www.mdpi.com), and precipitation/ion-exchange polishing out the rest, plants prepare a catholyte fit for high-purity electrowinning.

Bleed streams for impurity control

No chemical step removes all impurities permanently, so practical circuits rely on a controlled bleed (purge) stream to carry off accumulating metals. Any impurity that survives SX or precipitation — such as trace Ni, Co, Bi, or non-precipitated salts — will build up in a closed electrolyte loop. A small continuous bleed (typically on the order of <1–5% of the electrolyte flow per unit time) flushes these away. Industry sources imply that even very low bleed fractions are needed: if only 0.1% of the electrolyte is replaced per hour, a metal at 1 ppm in feed would accumulate to 7.2 ppm in 30 days without bleed. In practice, managing heavy metals (Ni, Zn, etc.) typically requires on the order of 0.1–0.5% daily bleed in a large plant. Without such bleed, even selective SX (which leaves some impurities) would eventually allow contaminants to reach critical levels.

This strategy is well-established beyond copper. In gold cyanidation, it is standard to bleed part of the carbon-adsorption eluate or barren liquor so that Cu and Pb levels stay “tolerable” (www.scirp.org). “It is always necessary to bleed some of the leach solution to maintain a tolerable level of impurity ions like copper and lead” when recycling cyanide solutions; the spilled (“bleed”) solution — high in cyanide and metals — must then be properly detoxified or precipitated before disposal (www.scirp.org).

Maintaining a bleed also underpins compliance. In Indonesia and elsewhere, environmental rules set strict discharge limits for heavy metals and cyanide in effluents. Indonesian standards (PP 82/2001 and related PermenLH) typically limit Cu, Zn, Ni to single-digit mg/L in wastewater. Regular bleeding and treatment of electrolyte streams help mines meet these limits, by preventing concentration of pollutants.

Bottom line: design for purity, design for purge

Copper and gold EW processes employ rigorous purification and bleed strategies. Copper SX–EW uses selective extractants and polishing precipitation (e.g., Fe removal by goethite/jarosite) to deliver high-purity Cu (SFU >95%) (www.mdpi.com). Gold/CN circuits use heavy‑metal precipitation (e.g., Zn dust, sulfide) to strip out Cu, Zn, Pb with >99% efficiency (file.scirp.org). Critically, a continuous bleed of the electrolyte loop (as practiced in industry, www.scirp.org) purges residual contaminants that chemical processes do not eliminate. Data-driven limits — Cu:Fe>6 (blog.emew.com) and Cl⁻<50 ppm (blog.emew.com) — keep electrowinning safe, efficient, and within environmental guardrails.

Sources: Industry and academic studies of SX–EW and gold leaching processes (blog.emew.com) (file.scirp.org) (link.springer.com) (www.scielo.org.za) (www.mdpi.com) (www.scirp.org). (All values and recommendations are drawn from these references.)