WhatsApp
By Marcus Somadjaja

When Ore Fights Back: How Carbon and Carbonates Hijack Gold and Copper Leaching — and What Actually Works

  • beta-pramesti-asia
  • industry-gold-dan-copper-mining
  • process-leaching-cyanide-for-gold-acid

When Ore Fights Back: How Carbon and Carbonates Hijack Gold and Copper Leaching — and What Actually Works

Preg-robbing carbon in gold ore can drain a few percent to over 50% of value, while acid-hungry carbonates in copper heaps can burn through reagent budgets. New and classic pretreatments show where miners win — and where they waste.

Industry: Gold_&_Copper_Mining | Process: Leaching_(Cyanide_for_Gold,_Acid_for_Copper)

Some rocks simply refuse to give up their metals. In gold, “preg-robbing” carbonaceous ores can sequester dissolved gold-cyanide complexes before plants can recover them — a loss that ranges from a few percent to over 50% of potential yield (researchgate.net). In copper, even minor shifts in gangue mineralogy can multiply sulfuric acid consumption and hobble leach kinetics (mdpi.com).

The fix is not a single reagent, but a toolkit. From flotation and roasting to biological oxidation and surfactant-aided leaches, operators are assembling flowsheets that neutralize these ore-specific traps — and, in regulated environments like Indonesia, curb cyanide and acid discharge (researchgate.net; iea.org).

Gold ore carbon and preg-robbing

Preg-robbing (adsorption of dissolved gold complexes onto native or biogenic carbon in ore) strips gold from pregnant solution. Carbon sources include humic substances and graphitic carbon; adsorption capacities span 30–65 g Au per tonne for low-grade wood to 580–650 g/t for active (graphitic) carbon over 24 hours (researchgate.net). Even small carbon fractions can “rob” many ounces into tails, “ultimately lowering the overall efficiency of the recovery process” (mdpi.com; mdpi.com). By contrast, silica/silicate gangue shows negligible preg-robbing (mdpi.com).

Extraction losses and lab evidence

Untreated refractory ore in one Colombian study yielded just 28.7% gold extraction; after bacterial bio-oxidation, extraction rose to 75–80% (researchgate.net). Lab tests show additive-sensitive behavior: protonated activated carbon (PAcC) can capture essentially all leached gold (up to 99.87%), whereas inert graphite caught only ~66% (mdpi.com). Plant-scale diagnoses commonly find missing gold in tails and dropping grades where preg-robbing is present; failing to mitigate typically leaves 10–50% or more of a gold ore’s value behind.

Gold pretreatment options and trade-offs

Flotation of carbonaceous matter physically removes the problem ahead of cyanide leach. Work with frother MIBC (methyl isobutyl carbinol) at 30–150 g/t and kerosene showed improved recovery and selectivity of carbonaceous matter in flotation (researchgate.net). In practice (e.g., Goldstrike, NV), carbon-rich froth concentrate is roasted to combust carbon, while carbon-depleted tails proceed to oxidation or direct leach (mdpi.com).

Oxidative pretreatments “bleach” carbonaceous matter. Roasting at ~650 °C for 2 hours in air created a porous matrix and yielded ~92.6% recovery on subsequent cyanidation (pubs.acs.org). Bio-oxidation with Acidithiobacillus spp. also degrades sulfides and passivates carbon; the same Colombian ore jumped from 28.7% to 75–80% extraction after bio-oxidation, with XRD/SEM showing oxygen group formation and C–C bond breakage that eliminated active adsorption sites (researchgate.net).

Reagent tactics include blanking agents that occupy carbon surfaces. Naphthalene sulfonate at 4.48 mM on a high-carbon ore (87% preg-robbing index) raised CIL (carbon-in-leach) recovery from 57% to 80% (researchgate.net). Plants often source these reagents as part of standard chemicals for mining programs.

Operating CIL/CIP (carbon-in-leach / carbon-in-pulp) with excess fresh carbon directs dissolved gold onto added adsorbent rather than native ore carbon; PAcC can take up ~99.9% of gold, and even anthracite (“inert” carbon) will capture about two-thirds when appropriately dosed (mdpi.com). Plants specify high-surface-area media such as activated carbon to execute this tactic. These pretreatments dramatically open locked gold to lixiviants, at the cost of heat or time; overall, roasting or bio-oxidation has taken recoveries from <30% to >90% in published cases (researchgate.net; pubs.acs.org).

Regulatory note: In Indonesia, cyanide leaching is tightly controlled; Minister of Environment Regulation No. 23/2008 governs cyanide use, and processors must capture or detoxify cyanide (researchgate.net). Managing preg-robbing (and thus cyanide consumption) improves yields and reduces discharge.

Acid-consuming gangue in copper heaps

In copper hydrometallurgy, especially heap leaching of oxide/secondary ores, “acid-consuming” gangue neutralizes sulfuric acid and slows copper dissolution. Carbonates — calcite, dolomite/ankerite, kutnahorite — are most notorious. A review notes that “even minor changes in gangue mineralogy can considerably impact acid consumption and copper recovery” (mdpi.com). Significant carbonate is often avoided because it “will dissolve completely in even very dilute sulfuric acid,” consuming acid with little Cu benefit (mdpi.com).

Operationally, acid-neutralizing gangue forces higher acid addition and can precipitate secondary minerals. Calcite develops a surface layer that clogs pores and precipitates gypsum/jarosite, dropping local pH; it “reacts quickly in acid,” slowing leach rates (researchgate.net). Iron-silicates and clays (biotite, chlorite) are less reactive short term but drive long-term acid consumption; one model flagged biotite and chlorite as key long-term drivers in porphyry ore (researchgate.net). Heap leaching is ≈21% of global Cu production, but recoveries are “often not optimal” due to such obstacles (mdpi.com).

Copper pretreatment and circuit adjustments

Where ore allows, beneficiation removes gangue ahead of leaching. Reverse flotation or density separation can strip calcite/dolomite. In Cu tailings high in CaO, a reverse-flotation circuit sent 71.6% of CaO (grade ~3.84% CaO) and 79.8% of Cu (0.82% Cu) to the floated concentrate (scientific.net). Another route roasts carbonate to CaO (~800–1000 °C), then uses low‑intensity magnetic separation (LIMS) to remove it; a review notes that such roast–LIMS significantly reduced downstream acid consumption by removing most Ca (researchgate.net).

Chemical/catalytic aids can target silicate gangue. Using CTAB (cetyltrimethylammonium bromide, a cationic surfactant) at 75 g/t during sulfuric acid leach of cupriferous mica increased Cu extraction from ~75% to 78.3% while slashing leach time by ~57% (80 minutes) (mdpi.com). The surfactant neutralized anionic layers in biotite, widening interlayers for acid attack; associated energy savings were estimated at $6–9 per ton. Other pretreats such as CaF2 and oxidants or chloride have been tested; CaF2 can significantly break down mica but risks introducing impurities (mdpi.com). These reagents sit squarely in the realm of standard chemical additives for hydromet circuits.

Concurring with Indonesia’s environmental rules (see below), operators typically neutralize excess gangue via lime or pre-washes. Leach pads may be initially wetted with weak acid to dissolve carbonates, then flushed before the main acid feed; ore is agglomerated with binders to maintain permeability through fines released by dissolving gangue. Geometallurgical prediction of acid demand often uses a rule of thumb of 12–15 kg H₂SO₄ per tonne feed in agglomeration (adjusted by gangue assay) (researchgate.net).

Regulatory context and water handling

Indonesia’s Ministry of Environment & Forestry Regulation No. 5/2022 mandates constructed-wetland treatment of mining wastewater (including copper and nickel leachate) before discharge, reflecting the need to neutralize residual acid and metals (iea.org). Earlier, cyanide use in gold processing was regulated by Minister of Environment Regulation No. 23/2008, requiring capture or detox of cyanide (researchgate.net).

Source links

Authoritative studies, including recent research and industry cases: mdpi.com; researchgate.net; pubs.acs.org; researchgate.net; mdpi.com; mdpi.com; researchgate.net; scientific.net; mdpi.com; researchgate.net; iea.org. Additional inline context: mdpi.com; mdpi.com; mdpi.com; mdpi.com; mdpi.com; researchgate.net; researchgate.net.